EN-GJS-600-3 | 5.3201 | Graphite classification and fracture appearance in tensile test
Numeric designation | 5.3201 |
---|---|
Chemical designation | EN-GJS-600-3 |
State | Graphite classification and fracture appearance in tensile test |
Etching | 3% Nital |
The microstructure of this ductile iron consists of >95% pearlite. The minimum tensile strength is 600 MPa, the minimum elongation at fracture 3%.
Graphite classification according to EN ISO 945-1:2019
- Graphite form VI
- Guide number for size range: 6
The SEM images show a force fracture by tensile testing. A transcrystalline cleavage fracture is present.