EN GJSA-XNi35
Numeric designation | EN-JS3051 |
---|---|
Chemical designation | EN GJSA-XNi35 |
Etching | Kalling 2 |
The fracture surface of the tensile specimen shows ductile fracture honeycombs in which the graphite spheres are located. The highly nickel-alloyed matrix could hardly be etched; Figure 10 shows examples of a few grain boundaries and the suggestion of a dendrite structure.
- Graphite classification according to DIN EN ISO 945-1 (2019): Form VI, size 6
- Tensile strength Rm approx. 450 MPa
- Rp0.2 approx. 245 MPa
- Elongation at break approx. 23 %
- KV 22 J at -196 °C
Note:
Hot V2A pickling eats a relief into the sample, next to which the few grain boundaries are barely visible.
Semi-concentrated HCl/H2O2 reacts violently, but only produces etching pits and ugly relief structures!